Hastelloy X UNS N06002 is a nickel-chromium-iron-molybdenum alloy known for its excellent high-temperature strength and oxidation resistance.
Hastelloy X Heat treatment is often used to optimize its mechanical properties, relieve stress from manufacturing processes, or improve its performance at elevated temperatures.
1. Solution Annealing (Primary Thermal Process)
Solution annealing is the most critical heat treatment for Hastelloy X, designed to dissolve secondary carbides and homogenize the microstructural grain matrix.
Temperature Range: Typically performed between 2150°F and 2250°F (1177°C to 1232°C).
Soaking Time: Dependent on section thickness and component mass, ranging from 30 minutes to several hours to ensure uniform heat penetration throughout the material cross-section.
Quenching Method: Rapid cooling-often via water quenching or rapid air/gas cooling (depending on thickness)-is mandatory immediately after soaking. Rapid quenching prevents unwanted secondary phase precipitation and preserves the ideal solid-solution microstructure.
2. Stress Relief Annealing (Post-Fabrication)
Components that undergo extensive cold working, forming, or heavy welding operations accumulate high internal residual stresses that can lead to distortion or cracking during service.
Temperature Range: Usually heated between 1600°F and 1900°F (871°C to 1038°C).
Cooling: Slow furnace cooling or controlled cooling is applied to safely relax internal stresses without fully altering the primary grain structure.
3. Post-Heat Treatment Surface Finishing
High-temperature thermal processing invariably produces surface oxides and scaling. To restore corrosion resistance and ensure clean surface integrity, components undergo:
Acid Pickling: Chemical baths to strip away high-temperature scale.
Passivation / Cleaning: Removing free iron and surface contaminants prior to deployment in corrosive industrial environments.
Summary Table: Hastelloy X Thermal Parameters
| Heat Treatment Type | Target Temperature Range | Primary Objective |
| Solution Annealing | 2150°F – 2250°F (1177°C – 1232°C) | Maximize high-temperature creep strength and homogenization |
| Stress Relief | 1600°F – 1900°F (871°C – 1038°C) | Relieve cold-working or welding residual stresses |
International Standards & Material Specifications
When specifying Hastelloy X components and their heat-treated conditions, refer to the following global standards:
| Material Form | ASTM Specification | ASME Specification | UNS / EN / DIN |
| Seamless & Welded Pipe/Tube | ASTM B619 / B622 / B626 | SB619 / SB622 / SB626 | UNS N06002 / W.Nr. 2.4665 |
| Plate, Sheet & Strip | ASTM B435 | SB435 | UNS N06002 / 2.4665 |
| Forgings & Bar | ASTM B572 | SB572 | UNS N06002 / 2.4665 |
| Fittings & Flanges | ASTM B366 | SB366 | UNS N06002 / 2.4665 |
Frequently Asked Questions & Troubleshooting
Q1: Can Hastelloy X be age-hardened or precipitation-hardened?
No. Hastelloy X is a solid-solution strengthened alloy. It cannot be hardened by heat treatment/aging. High strength is achieved through molybdenum, chromium, and cobalt solid-solution effects and work hardening.
Q2: What happens if Hastelloy X is cooled slowly after annealing?
Slow cooling through the 1200°F to 1800°F (650°C to 980°C) range leads to precipitate formation along grain boundaries, which reduces ductility and room-temperature impact toughness.