Mar 14, 2024 Leave a message

17-4PH Stainless Steel (AISI 630 / 1.4542): Properties, Heat Treatment & Applications

 

Four names for one alloy, and only one is safe on a PO

17-4PH, AISI 630, 1.4542 and UNS S17400 all describe the same precipitation-hardening stainless steel. Three of those names are ambiguous in practice; UNS S17400 is not, which is why it belongs on the purchase order even when the drawing uses a trade name.

 

 

AISI 630 is the older US designation and says nothing about condition. 1.4542 is the EN number and carries a European chemistry tolerance set. 17-4PH is a trade name owned by nobody in particular, so any mill can print it.

 

 

Table 1. Chemical composition, UNS S17400 (17-4PH / AISI 630 / 1.4542)

Element Range (wt%) Role
C 0.07 max toughness
Mn 1.00 max deoxidation
Si 1.00 max deoxidation
P 0.040 max trace limit
S 0.030 max trace limit
Cr 15.0 - 17.5 passive film
Ni 3.0 - 5.0 austenite balance
Cu 3.0 - 5.0 the hardener
Nb + Ta 0.15 - 0.45 (5 x C min) grain control
Fe balance matrix

 

 

The name problem matters most at the ageing step, because the same alloy in three conditions gives three unrelated property sets.

 

 

Table 2. Mechanical minimums by condition, bar and forgings

Condition UTS min 0.2% YS min Elong. in 2 in Hardness HRC
H900 1310 MPa (190 ksi) 1170 MPa (170 ksi) 10% 40 min
H1025 1070 MPa (155 ksi) 1000 MPa (145 ksi) 12% 35 min
H1150 930 MPa (135 ksi) 724 MPa (105 ksi) 16% 28 min

 

Reading a certificate that mixes naming systems

H900 is the strength condition: actuator rods, valve stems, high-load fasteners. Rough machine before ageing, finish after - 40 HRC is unforgiving.

 

H1025 is the structural compromise. Around 10% less yield than H900, better ductility and fatigue life, and normal machining practice still works.

 

H1150 is the corrosion-driven choice for chloride service, where stress corrosion cracking rather than load sets the limit.

 

 

The practical rule: quote UNS S17400 plus the condition plus the product form. A PO that says "17-4PH" alone leaves the mill free to ship any of the four naming variants and any condition. Ask us to cross-check the standard numbers on your drawing.

 

Alloy 17-4PH / 630 / 1.4542 stainless steel supplier, contact us to get free quote and sample!

 

What is 17-4PH, 1.4542, AISI 630 stainless steel?

Alloy 17-4PH / 630 / 1.4542 stainless steel is one of the most popular and most commonly used stainless chromium-nickel alloy steels with copper additive, precipitation hardened with martensitic structure. Steel can operate in the temperature range from -29 ℃ to 343 ℃, while retaining relatively good parameters. In addition, the materials in this grade are characterized by relatively good ductility and their corrosion resistance is comparable to 1.4301 / X5CrNi18-10.

 

AISI 630 Stainless Steel pipe

 

AISI 630 Stainless Steel Properties

AISI 630 stainless steel is one of the newest stainless steel grade found in 1960s. This grade is written as 1.4542 or X5CrNiCuNb16-4 or 17-4 PH according to EN norm and it is written as UNS S17400 according to UNS norm. DIN 1.4542 material is a very special grade because of its mechanical properties. The yield and tensile strenght are usually both higher then 1000MPA and if we compare this grade with the most famous grade 304, then we can understand how strong this grade is. In 304 grade, the yield is about 300MPA but in 630 (1.4542) the yield is over 1000MPA.

 

Alloy 630 (17Cr-4Ni) is a martensitic precipitation/age-hardening stainless steel offering high strength and hardness along with excellent corrosion resistance. It has good fabricating characteristics and can be age hardened by a single-step, low temperature treatment. It has been used for a variety of applications including oil field valve parts, chemical process equipment, aircraft fittings, fasteners, pump shafts, nuclear reactor components, gears, paper mill equipment, missile fittings, and jet engine parts.

 

17-4PH Stainless Steel Pipe is a precipitation hardening stainless steel and because of precipitation hardening, it is also called PH 17-4 or 17-4 PH. SUS 630 stainless steel materials usually in three different heat threatment conditions. The most common one is H1025 heat threated version. H1025 heat threat version usually has a tensile strenght above 1100 MPA and hardness above 37 HRC. The other heat threatment conditions are Condition A, which is not precipitated yet and H1150, which is softened and has a lower hardness and lower mechanical value. 

 

AISI 630 Stainless Steel Heat Treatment:

Solution Annealing (Condition A):
The alloy is heated to a high temperature (around 1010°C to 1065°C) and held for a sufficient time to dissolve any precipitated phases. This step aims to homogenize the alloy's microstructure.

 

Quenching:
After solution annealing, the alloy is rapidly cooled (quenched) to room temperature, usually in water or oil, to retain the dissolved elements in a supersaturated solid solution.

 

Precipitation Hardening (Aging):
The quenched alloy is then subjected to aging at a moderately elevated temperature (typically around 480°C to 620°C) for a specific duration. During this process, precipitation of fine particles (usually copper-rich phases) occurs within the matrix, leading to the desired strengthening effect.

 

Tempering (Optional):
In some cases, a tempering step may follow precipitation hardening to further adjust the mechanical properties and improve toughness.

Contact now

 

 

 

 