ASTM A213 Standard
ASTM A213 standard is a common used specification for Seamless Ferritic and Austenitic Alloy-Steel Boiler, Super heater, and Heat-Exchanger Tubes, offering manufacture and purchasing requirements for manufactures and users, main information contain grade, size, finishes, test and other terms, the equivalent standard is ASME SA213.
ASTM A213 Standard Grades
ASTM A213 Stainless Steel Tube specification contains many grades, alloy grades are mainly T5, T9, T11, T12, T22, T91, stainless grades are 304, 304L, 316, 316L, 316Ti, 316L Mod, 17-4ph, 310, 310S, 317, 317L, 321, 321H, 347, 347H, 904L, 254SMO, 253MA, S32550, S32205, S31803, 2507, S31050, S30815 for more grades.
Chemical Composition Of ASTM A213 Stainless Steel Tubes
| Steel Grades | ASTM A213 Chemical Composition % Max | ||||||||||
| C | Mn | P | S | Si | Cr | Ni | Mo | NB | Nb | Ti | |
| TP304 | 0.08 | 2.00 | 0.045 | 0.030 | 0.75 | 18.0-20.0 | 8.0-11.0 | … | … | … | … |
| TP304H | 0.04-0.10 | 2.00 | 0.040 | 0.030 | 0.75 | 18.0-20.0 | 8.0-11.0 | … | … | … | … |
| TP304L | 0.035 | 2.00 | 0.040 | 0.030 | 0.75 | 18.0-20.0 | 8.0-13.0 | … | … | … | … |
| TP310S | 0.08 | 2.00 | 0.045 | 0.030 | 0.75 | 24.0-26.0 | 19.0-22.0 | 0.75 | … | … | … |
| TP310HCbN | 0.04-0.10 | 2.00 | 0.030 | 0.030 | 0.75 | 24.0-26.0 | 17.0-23.0 | … | 0.15-0.35 | 0.20-0.60 | … |
| TP316 | 0.08 | 2.00 | 0.040 | 0.030 | 0.75 | 16.0-18.0 | 11.0-14.0 | 2.00-3.00 | … | … | … |
| TP316L | 0.035 | 2.00 | 0.040 | 0.030 | 1.00 | 16.0-18.0 | 10.0-15.0 | 2.00-3.00 | … | … | … |
| TP316H | 0.04-0.10 | 2.00 | 0.040 | 0.030 | 0.75 | 16.0-18.0 | 11.0-14.0 | 2.00-3.00 | … | … | … |
| TP321 | 0.08 | 2.00 | 0.040 | 0.030 | 0.75 | 17.0-20.0 | 9.0-13.0 | … | … | … | 5C-0.60 |
| TP321H | 0.04-0.10 | 2.00 | 0.040 | 0.030 | 0.75 | 17.0-20.0 | 9.0-13.0 | … | … | … | 4C-0.60 |
| TP347 | 0.08 | 2.00 | 0.040 | 0.030 | 0.75 | 17.0-19.0 | 9.0-13.0 | … | … | 10xC-1.00 | … |
| TP347H | 0.04-0.10 | 2.00 | 0.040 | 0.030 | 0.75 | 17.0-20.0 | 9.0-13.0 | … | … | 8xC-1.00 | … |
Mechanical Properties Of ASTM A213 Stainless Steel Tubes
| Steel Grades | Heat Treatment | Temperure F (C) Min. | ASTM grain size NO. | Tensile Strength Ksi (MPa), Min. | Yield Strength Ksi (MPa), Min. | Elongation %, Min | Hardness | |
| Brinell | Rockwell | |||||||
| TP304 | Solution | 1900 (1040) | … | 75(515) | 30(205) | 35 | 192HBW/200HV | 90HRB |
| TP304L | Solution | 1900 (1040) | … | 70(485) | 25(170) | 35 | 192HBW/200HV | 90HRB |
| TP304H | Solution | 1900 (1040) | 7 | 75(515) | 30(205) | 35 | 192HBW/200HV | 90HRB |
| TP310S | Solution | 1900 (1040) | … | 75(515) | 30(205) | 35 | 192HBW/200HV | 90HRB |
| TP310HCbN | Solution | 2000 (1110) | 7 | 95(655) | 43(295) | 30 | 256HBW | 100HRB |
| TP316 | Solution | 1900 (1040) | … | 75(515) | 30(205) | 35 | 192HBW/200HV | 90HRB |
| TP316L | Solution | 1900 (1040) | … | 70(485) | 25(170) | 35 | 192HBW/200HV | 90HRB |
| TP316H | Solution | 1900 (1040) | 7 | 75(515) | 30(205) | 35 | 192HBW/200HV | 90HRB |
| TP321 | Solution | 1900 (1040) | 7 | 75(515) | 30(205) | 35 | 192HBW/200HV | 90HRB |
| TP321H | Solution | 2000(1100) | 7 | 75(515) | 30(205) | 35 | 192HBW/200HV | 90HRB |
| TP347 | Solution | 1900(1040) | … | 75(515) | 30(205) | 35 | 192HBW/200HV | 90HRB |
| TP347H | Solution | 2000(1100) | 7 | 75(515) | 30(205) | 35 | 192HBW/200HV | 90HRB |
ASTM A213 Tolerances, Outside Diameter, Wall Thickless And Length
The SA213 tubing sizes and thicknesses usually furnished to this specification are 1/8 inch [3.2 mm] in inside diameter to 5 inch [127 mm] in outside diameter and 0.015 to 0.500 in. [0.4 to 12.7 mm]. Custom outside diameter and wall thickness, tubing having other diameters may be furnished.
ASME SA213 tubing Wall Thickness Tolerances
ASTM A213 specifies Minimum wall thickness, namely, there is no mill undertolerance, only overtolerance, unless specified as average wall thickness is requied, permissible variations from the specified average wall thickness shall be +/-10 % of the specified average wall thickness for cold formed tubes. ASME SA213 stainless steel tubing furnished to this specification shall conform to the requirements of Specification ASTM A1016/A1016M.
Cold Finished Seamless Tubes
| OD | OD Tolerance | OD Tolerance | WT Tolerance | WT Tolerance | Length Tolerance | Length Tolerance |
|---|---|---|---|---|---|---|
| Mm | Over | Under | Over | Under | Over | Under |
| Under 25.4 | 0.1016 | 0.1016 | +20 | -0 | 3.175 | 0 |
| 25.4-38.1 Incl | 0.1524 | 0.1524 | +20 | -0 | 3.175 | 0 |
| 38.1-50.8 Excl | 0.2032 | 0.2032 | +22 | -0 | 3.176 | 0 |
| 50.8-63.5 Excl | 0.254 | 0.254 | +22 | -0 | 4.46 | 0 |
| 63.5-76.2 Excl | 0.3048 | 0.3048 | +22 | -0 | 4.76 | 0 |
| 76.2-101.6 Incl | 0.381 | 0.381 | +22 | -0 | 4.76 | 0 |
| 101.6-190.5 Incl | 0.381 | 0.635 | +22 | -0 | 4.76 | 0 |
| 190.5-228.6 Incl | 0.381 | 1.143 | +22 | -0 | 4.76 | 0 |
Hot Finished Seamless Tubes OD Tolerance
| Outside Diameter, Mm | Tolerance, Mm |
|---|---|
| OD≤101.6 | +0.4/-0.8 |
| 101.6<OD≤190.5 | +0.4/-1.2 |
| 190.5<OD≤228.6 | +0.4/-1.6 |
Hot Rolled Wall Thickness Tolerance
| Outside Diameter, Mm | Tolerance, % |
|---|---|
| OD≤101.6, WT≤2.4 | +40/-0 |
| OD≤101.6, 2.4<WT≤3.8 | +35/-0 |
| OD≤101.6, 3.8<WT≤4.6 | +33/-0 |
| OD≤101.6, WT>4.6 | +28/-0 |
| OD>101.6, 2.4<WT≤3.8 | +35/-0 |
| OD>101.6, 3.8<WT≤4.6 | +33/-0 |
| OD>101.6, WT>4.6 | +28/-0 |
ASTM A213 Seamless Tubing Manufacturing Processes
- The tubes shall be made by the seamless process and shall be either hot finished or cold finished, as specified.
- Heat treatment shall be done separately and in addition to heating for hot forming.
- The ferritic alloy and ferritic stainless steels shall be reheated. austenitic stainless steel tubes shall be furnished in the heat-treated condition.
- Tubes may be individually quenched in water or rapidly cooled by other means.
- Tubes shall be pickled free of scale. When bright annealing is used, pickling is not necessary.
- Complete tests should be conducted conforming to ASTM A213 or ASTM A1016.
A213 Stainless Steel Tubing Testing Requirement
Each tube shall be subjected to the nondestructive electric test or hydrostatic test, Manufacturer Material Test Certification as per EN 10204 3.1 should be provided.
- Tensile property, Elogation
- Hardness testing, Brinell, Rockwell, Vickers hardness
- Flattening testing
- Flaring testing
- Hydrostatic or Nondestructive test
- Intergranular Corrosion Test – ASTM A262/E (option)