Sep 29, 2026 Leave a message

ASTM B168 Alloy 600 Plate: High-Temperature Strength and Where It Fails

A heat-treatment furnace engineer checks the datasheet for a new batch of radiant-tube support plates. The room-temperature numbers are unremarkable - 655 MPa tensile, 310 MPa yield - about what you would expect from a decent stainless grade. Then the engineer scrolls to the 1000 C row and stops: 175 MPa tensile, 140 MPa yield, 55% elongation. At that temperature 316L plate has collapsed to roughly a quarter of its room-temperature strength and is creeping visibly.

 

Inconel 600 plate is still holding load. The question is not whether the numbers are real - they are, and they are in every B168 certificate. The question is why, because the answer decides whether 600 is the right plate for your furnace, and whether it is the wrong plate for the atmosphere inside it.

Product Forms

Bar & Rod

Plate & Sheet

Coil & Strip

Pipe & Tube

Fitting: Flange, Tee, Elbow, Reducer etc.

Forging: Ring, Shaft, Circle, Block etc.

inconel 600 plate

The 72-14-6 Formula: What Each Number Does

Element Content What it does on the plate
Nickel (Ni) 72.0% min The matrix. Face-centred-cubic austenite, stable from cryogenic to melt. No phase transformation means no embrittlement window, and 72% Ni is the threshold for chloride stress-corrosion cracking immunity.
Chromium (Cr) 14.0-17.0% The oxidiser. Forms Cr2O3 above about 800 C; below that the oxide is thin and protective. This row sets the upper-temperature oxidation limit and the sulfidation vulnerability.
Iron (Fe) 6.0-10.0% Solid-solution strengthener and cost reducer. Replaces expensive Ni while maintaining the FCC matrix; does not form hardening precipitates.
Carbon (C) 0.15% max Kept low enough to avoid chronic sensitisation, high enough (0.05-0.10% typical) to give modest carbonitride pinning that stabilises grain size during long furnace exposure.
Manganese / Silicon (Mn / Si) 1.0 / 0.5 max Deoxidation and melting discipline; Si in particular affects oxide adhesion during thermal cycling.
Sulfur (S) 0.015% max Tight control - sulfur is the enemy of high-temperature nickel alloys.

 

Notice what is not in the table: aluminium, titanium, niobium, molybdenum. Those are the elements that make precipitation-hardened nickel alloys (718, 625 in its aged condition, X-750) and the elements that give 625 its PREN of 51. Their absence from 600 is not a cost shortcut - it is a design decision. 600 plate is a solid-solution alloy, full stop. That decision shapes everything that follows.

 

Solid-Solution Strengthening: The Only Game in Town

In precipitation-hardenable nickel alloys, strength comes from ordered intermetallic phases - gamma prime (Ni3(Al,Ti)) or gamma double-prime (Ni3Nb) - that pin dislocations. Heat-treat the plate, the precipitates form, the strength jumps. Inconel 600 plate contains no Al and no Ti, so no gamma prime forms. There is no heat-treatment trick that will raise its yield from 310 MPa to 600 MPa. The only way to strengthen 600 plate is to cold-work it - roll it thinner, draw it, stamp it - and let dislocation density do what precipitates cannot.

 

Condition Tensile (MPa) Yield (MPa) Elongation How it is achieved
Annealed (soft) 550-690 240-345 30-55% Recrystallised at about 1050 C; lowest strength, best formability
Quarter-hard About 760 About 620 20-25% Cold reduction about 10-15%
Half-hard About 860 About 760 10-15% Cold reduction about 20-30%
Full-hard About 965 About 860 5-10% Cold reduction about 35-45%

 

For plate buyers, this means two things. First, if your design needs yield above about 350 MPa at temperature, you must specify a cold-worked temper or move to a different alloy (625, 800HT).

 

Second, annealed 600 plate is chosen for its creep and oxidation resistance, not its strength. A furnace builder ordering radiant-tube hanger plates for a 950 C carburising line does not buy 600 for its yield; they buy it because the microstructure of the alloy is still single-phase austenite at that temperature, with no precipitates to over-age and no phase boundaries to embrittle.

 

The Oxide Skin: Cr2O3, NiO and the Temperature Hand-Over

When 600 plate heats in air, it grows an oxide. Below roughly 800-850 C the scale is thin, adherent and dominated by chromium oxide (Cr2O3) - the same protective film that makes stainless steels stainless. Above that band the scale thickens, nickel oxide (NiO) becomes a significant outer layer, and the protection becomes less perfect. The transition is gradual, not sudden, but it matters for plate life:

 

Temperature band Dominant oxide Appearance / consequence
Up to about 800 C Cr2O3 (thin) Dark, adherent, protective - the plate behaves like a high-nickel stainless
800-1000 C Cr2O3 + NiO duplex Scale thickens, may spall on thermal cycling; weight-gain accelerates
Above about 1000 C NiO-rich outer layer Faster growth; design for extra wall or shorter inspection interval

 

This is why 600 plate is specified with a corrosion allowance even in "clean" oxidising furnace service: the scale consumes metal, and over a five-year campaign the cumulative loss is measurable. The rate is far slower than carbon steel or even 310S, but it is not zero.

 

Where 600 Plate Quietly Fails: Sulfur and Carbon

Here is the knowledge gap the SERP never covers. Cr2O3 is not protective in sulfidising or strongly reducing carburising atmospheres. In a heat-treatment furnace running cracked ammonia, endothermic gas, or any atmosphere with even ppm-level sulfur, the chromium oxide is destabilised. Sulfur penetrates the scale, forms chromium sulfide (Cr2S3) beneath it, and the oxide ceases to be a barrier. The nickel matrix is then exposed to direct attack, and the attack is rapid - sulfidation of nickel alloys proceeds orders of magnitude faster than oxidation in air.

 

Atmosphere Verdict Why
Clean air / oxidising combustion Excellent Cr2O3 stable and protective
Slightly oxidising, low sulfur Good Thin scale, acceptable metal loss
Reducing, carburising (endogas, CH4-rich) Caution Carburisation risk; carbon ingress can embrittle surface unless the plate is pre-oxidised or the atmosphere controlled
Sulfidising (H2S, SO2, cracked fuel with S) Poor Cr2O3 destroyed; sulfidation rate high - consider 625 or HR-160 for sulfur duty
Alternating oxidising / reducing (thermal cycling) Moderate Scale spallation on cycling; design for thicker initial wall

 

The practical rule: if your furnace atmosphere contains sulfur, 600 plate is the wrong alloy regardless of its tensile strength at temperature. A heat-treatment shop running endothermic gas with trace sulfur learned this the hard way: 600 radiant tubes that lasted four years in clean air failed in eighteen months after a fuel switch. The replacement was not more 600 - it was 625, whose higher Cr and Mo content resists sulfidation far better.

 

The Boundary: When to Move to 625 or 800HT

 

Requirement 600 plate 625 plate 800HT plate
Max temperature, long-term About 1100 C About 1000 C About 1000 C
Strength driver Solid solution + cold work Solid solution + some gamma prime potential Solid solution + carbonitride creep resistance
Sulfur resistance Weak Strong (Mo + higher Cr) Moderate
Carburisation resistance Moderate Good Good (higher Ni, controlled C)
Price tier (plate) Baseline nickel +30-50% +10-20%
Typical plate use Furnace fixtures, radiant hangers, muffles Sulfur-containing furnace, chemical reactor cladding Petrochemical furnace tubes, creep-critical hangers

 

600 plate wins on cost and on the highest-temperature oxidising duties where strength is secondary. It loses to 625 the moment sulfur enters the atmosphere, and it loses to 800HT on creep-limited pressure parts where carbonitride strengthening controls deformation.

 

Reading the B168 Certificate for Plate

Three rows to audit beyond the usual chemistry and tensile:

 

  • Grain size: ASTM 5 or finer is typical for annealed plate; coarse grains (ASTM 2-3) improve creep resistance but reduce room-temperature toughness - know which side your application sits on.
  • Surface: No.1 (hot-rolled, oxidised) for furnace fixtures that will be machined; 2B or polished only if the plate faces a process fluid where surface finish affects fouling.
  • Flatness: B168 does not specify tight flatness; if you are laser-cutting fixture blanks, state flatness on the PO or budget for stress-relief before machining.

 

Frequently Asked Questions

Q: Can Inconel 600 plate be hardened by heat treatment?

 

A: No. Without Al or Ti there is no gamma prime phase to precipitate. The only strengthening route is cold work. For high-strength high-temperature plate, move to 625 or 718.

 

Q: What is the maximum service temperature for 600 plate?

 

A: Roughly 1100 C in clean oxidising air for short-term exposure; 980-1050 C for long-term structural load. Above 1000 C oxidation rate accelerates and scale spallation becomes the life limiter.

 

Q: Why does 600 plate resist chloride stress-corrosion cracking?

 

A: The 72% Ni minimum. SCC in chlorides is an austenitic-stainless problem; nickel alloys above about 45% Ni are effectively immune, and 600 is well above that threshold.

 

Q: Is 600 plate weldable?

 

A: Yes - fully austenitic, no preheat, no PWHT. Matching filler is ERNiCrFe-1 (FM 82/92 family) or ERNiCr-3. The weld metal will be softer than cold-worked base plate; design joints in annealed plate or accept the mismatch.

 

Q: How does 600 plate compare to 310S stainless in furnace service?

 

A: 600 has higher nickel and better thermal fatigue resistance; 310S is cheaper and adequate to about 1050 C in clean air. Where thermal cycling is severe or sulfur is present, the 600 nickel matrix wins - but 625 wins even more.

 

Send your furnace conditions - temperature, atmosphere composition, sulfur level, and load requirement - to market@htpipe.com. We will tell you whether annealed 600 plate is the right spend, whether cold-worked temper is worth the premium, or whether sulfur in your gas stream makes 625 the cheaper choice over the campaign life.

Contact now

 

 

Send Inquiry

whatsapp

Phone

E-mail

Inquiry